Alumina CTE (coefficient of thermal expansion) for our six standard grades is 7.7 to 8.4 × 10⁻⁶/°C, measured as a mean value from 25 to 800 °C. In everyday terms, a 100 mm alumina part grows about 0.6 mm between room temperature and 800 °C. Before you compare that with another datasheet, check the temperature interval, because it moves the number about as much as the grade does. One major supplier’s published 99% grade reads 7.2 × 10⁻⁶/°C over 40 to 400 °C and 8.0 over 40 to 800 °C. Same material, two values.
This guide gives the grade-by-grade values from our alumina QC data, shows how to read the interval on a datasheet, and walks through how to check expansion mismatch where alumina meets stainless steel, Kovar, copper, or silicon.
Alumina CTE by Grade
The spread across grades is narrow. The 99% and higher grades sit slightly below 95% and 97%.
| Grade | Mean CTE, 25 to 800 °C (× 10⁻⁶/°C) |
|---|---|
| 95% Al2O3 | 8.4 |
| 97% Al2O3 | 8.3 |
| 99% Al2O3 | 7.7 |
| 99.5% Al2O3 | 7.8 |
| 99.7% Al2O3 | 7.8 |
| 99.99% Al2O3 | 8.0 |
Values from our QC data.
The biggest step falls between 97% and 99%, where the value drops from 8.3 to 7.7. From 99% upward everything stays between 7.7 and 8.0.
For density, strength, and electrical values on the same six grades, see the data hub linked above. If you are still choosing a purity, our guide to alumina grades and what each one buys covers that decision.
Why Two Datasheets Give Different Alumina CTE Values
Usually they measured different temperature intervals, not different materials. The CTE on a ceramic datasheet is a mean coefficient: the total change in length between two temperatures, divided by the temperature difference. Alumina expands a little faster as it gets hotter. An interval that reaches a higher temperature therefore returns a larger mean value.
One supplier’s published data shows this clearly, with every grade tested over two intervals:
| Grade (published supplier data) | 40 to 400 °C | 40 to 800 °C |
|---|---|---|
| ≥96% Al2O3 | 7.2 | 7.9 |
| ≥99% Al2O3 | 7.2 | 8.0 |
| ≥99.7% Al2O3 | 7.2 | 8.0 |
Mean CTE in × 10⁻⁶/°C, measured to JIS R 1618.
Extending the interval from 400 to 800 °C adds 0.7 to 0.8 to every grade on that sheet. Across our six grades, the gap between the highest and lowest value is 0.7. So switching intervals can shift the figure at least as much as switching grades.
The two data sets also come close once the intervals line up. Our 99% reads 7.7 over 25 to 800 °C, and the supplier’s 99% reads 8.0 over 40 to 800 °C. Put our 7.7 next to their 7.2 at 400 °C, though, and it looks like a different material.
That is why figures quoted online vary so widely. Most are correct for their own interval. Many summaries simply drop the interval. Some references also publish an instantaneous coefficient, the expansion rate at a single temperature, which is not interchangeable with a mean value. Check which kind a datasheet shows.
Matching Alumina CTE to Metals and Silicon
Alumina sits between silicon and most structural metals, so nearly every joint carries some mismatch. What matters is its size over the temperature range the joint actually sees.
| Material | Mean CTE (× 10⁻⁶/°C) | Interval |
|---|---|---|
| Silicon | about 2.6 | Room temperature |
| Molybdenum | about 4.8 | Room temperature |
| Kovar (annealed) | 5.1 | 25 to 400 °C |
| Kovar (annealed) | 9.1 | 25 to 700 °C |
| Alumina 99% (published supplier data) | 7.2 | 40 to 400 °C |
| Alumina 99.5% (our QC data) | 7.8 | 25 to 800 °C |
| Copper | about 16.5 | Room temperature |
| 304 stainless steel | 16.9 | 0 to 100 °C |
| 304 stainless steel | 18.7 | 0 to 649 °C |
Metal and silicon values are typical published figures. Use the datasheet for your exact alloy, and compare it with the alumina value over the same interval.
Silicon expands at roughly a third of alumina’s rate, which is why die-attach layers on alumina substrates have to absorb strain during thermal cycling. Copper and austenitic stainless steel run at more than twice alumina’s rate, and since alumina’s value near room temperature is lower still, the real gap is wider. Molybdenum and Kovar are the close partners, and Kovar needs a closer look.
Kovar matches alumina only over part of the range
Kovar’s expansion curve is not straight. Its mean CTE stays between about 4.9 and 5.9 × 10⁻⁶/°C up to about 450 °C, then climbs steeply, because the alloy has passed its Curie point at about 435 °C. Below that, alumina expands more than Kovar. Somewhere between 500 and 700 °C the order reverses.
A room-temperature pair of numbers hides this reversal completely. When you check a Kovar joint, compare the two materials over the brazing cooldown and over the service range separately, because the mismatch runs in opposite directions in the two ranges. Over 25 to 700 °C Kovar already averages 9.1 × 10⁻⁶/°C, above alumina’s 7.7 to 8.0 measured all the way to 800 °C. The gap is still far smaller than with stainless steel. For the metallization routes used on these joints, see our alumina ceramic insulator guide.
Worked example: alumina brazed directly to 304 stainless steel
A quick estimate shows why direct ceramic-to-steel joints crack. Multiply the CTE gap by the temperature drop to get the mismatch strain, then compare it with how far alumina can stretch before it breaks.
Temperature drop. Silver-copper braze alloys solidify at about 780 °C, so the joint locks in near 780 °C and cools to 25 °C: a drop of 755 °C.
CTE gap. 304 stainless steel at 18.7 (0 to 649 °C, the widest interval in the published table) minus 99.5% alumina at 7.8 (25 to 800 °C) gives 10.9 × 10⁻⁶/°C. The steel’s true mean value up to 780 °C is a little higher, so this understates the gap.
Mismatch strain. 10.9 × 10⁻⁶ × 755 ≈ 0.0082, or 0.82%.
What alumina can absorb. Bending strength of 355 MPa (99.5%) divided by a published Young’s modulus of about 380 GPa for 99.7% alumina gives a failure strain of about 0.093%. The tensile limit is lower still.
Result. A fully rigid joint would ask the ceramic to absorb almost nine times its failure strain.
Real stresses depend on geometry and on how much the braze yields, so treat this as a scale check, not a stress analysis. The scale is the point. Published brazing practice puts a cushioning layer, such as molybdenum or Kovar, between alumina and a higher-expansion metal for this reason. For how stiffness varies by grade, see our guide to the Young’s modulus of alumina; our article on tensile and yield strength of alumina explains why the tensile limit sits below the bending value.
How to Specify Alumina CTE on a Drawing or RFQ
Ask for the mean CTE over the interval your part actually sees, and write that interval down. A useful specification covers four things:
- The interval. Give the process range (brazing or firing temperature down to room temperature) and the service range separately.
- Mean or instantaneous. State which one you need, so the supplier does not answer with the other.
- The grade and the test standard. Datasheets from Japanese suppliers may cite JIS R 1618; the standard tells you how the sample was heated and measured.
- The matching metal value over the same interval. A joint check is only as good as its least comparable number.
Our alumina CTE values are measured over 25 to 800 °C. If your joint or service range differs, send the joint materials and temperature profile with your drawing through our quote request form, and we will confirm the alumina grade and the CTE data we hold for it within 24 hours.
Frequently Asked Questions
Not within 99% to 99.99%, which sit between 7.7 and 8.0 × 10⁻⁶/°C over 25 to 800 °C in our data. The step that matters is from 95% or 97% (8.4 and 8.3) to 99% or above. That is minor against stainless steel, but recheck joints to close partners such as Kovar or molybdenum.
Not exactly. Sapphire is single-crystal Al2O3, so its expansion depends on direction. One published sapphire grade reads 7.7 × 10⁻⁶/°C parallel to the c-axis and 7.0 perpendicular to it over 40 to 400 °C, while the same supplier’s polycrystalline 99% alumina reads a single 7.2. Specify the crystal orientation for sapphire parts.
Alumina expands more than the nitride and carbide ceramics. On one supplier’s 40 to 400 °C data, silicon nitride reads 2.8, silicon carbide 3.7, and aluminum nitride 4.6 × 10⁻⁶/°C, against 7.2 for 99% alumina. That puts silicon nitride and aluminum nitride closer to silicon, while alumina sits between them and most structural metals.
CTE is one of several factors, with strength, stiffness, and thermal conductivity, that set thermal shock resistance: lower expansion means less strain when one side of a part heats faster. Alumina’s conductivity falls as it heats, which our thermal conductivity of alumina guide covers. All six of our grades pass a 25 to 800 °C thermal shock test.
References
- Kyocera Fineceramics Europe material datasheets: AO476O (≥96% alumina), AO479O (≥99%), and AO480S (≥99.7%); Kyocera, coefficient of thermal expansion by material, fine ceramics material catalog (sapphire by crystal axis), and property comparison (alumina Young’s modulus)
- High Temp Metals, Kovar technical data (mean coefficient of thermal expansion, annealed)
- Physical properties of stainless steel 304, mean coefficient of thermal expansion
- MISUMI, thermal expansion coefficients of metals (copper, molybdenum, silicon)
- US Patent 4,785,989, clad system for brazing to alumina
- Wesgo, Cusil silver-copper braze alloy technical data sheet (solidus and liquidus 780 °C)